Properties |
Standard |
Unit |
E175 |
E180 |
E185 |
E190 |
E195 |
E155D |
E165D |
E175D |
||
Density |
ASTM D792 |
g/cm3 |
1.18 |
1.19 |
1.19 |
1.19 |
1.2 |
1.21 |
1.21 |
1.22 |
||
Hardness |
ASTM D2240 |
Shore A/D |
74/- |
82/- |
86/- |
92/- |
95/- |
-/55 |
-/65 |
-/75 |
||
Tensile Strength |
ASTM D412 |
MPa |
22 |
35 |
40 |
45 |
50 |
52 |
55 |
60 |
||
100%Modulus |
ASTM D412 |
MPa |
3 |
5 |
7 |
10 |
15 |
16 |
22 |
35 |
||
300%Modulus |
ASTM D412 |
MPa |
7 |
12 |
15 |
24 |
35 |
38 |
40 |
43 |
||
Elongation at Break |
ASTM D412 |
% |
600 |
550 |
500 |
450 |
400 |
380 |
350 |
300 |
||
Tear Strength |
ASTM D624 |
kN/m |
75 |
100 |
120 |
140 |
160 |
180 |
200 |
240 |
||
DIN Abrasion Loss |
DIN 53516 |
mm3 |
/ |
30 |
30 |
35 |
35 |
35 |
35 |
40 |
||
Tg |
DSC |
℃ |
-42 |
-40 |
-37 |
-32 |
-30 |
-26 |
-22 |
-15 |
||
Compression Set |
22 hours @70℃ |
ASTMD395 |
% |
/ |
18 |
21 |
24 |
25 |
28 |
30 |
32 |
|
24 hours@100℃ |
ASTMD395 |
% |
/ |
28 |
30 |
33 |
35 |
36 |
38 |
40 |
Processing Guide for Injection Molding | Processing Guide for Extrusion | |||
Item | Parameter | Item | Parameter | |
Nozzle(℃) |
Given in the TDS |
Die(℃) | Given in the TDS | |
Metering Zone(℃) | Adapter(℃) | |||
Compression Zone(℃) | Metering Zone (℃) | |||
Feeding Zone(℃) | Compression Zone (℃) | |||
Injection Pressure(bar) | Feeding Zone (℃) |